Repairing a Bearing Housing In Situ with Brush Plating
Brush Plating Repair on a Bearing Housing
When a bearing housing wears, scores, or corrodes, the usual options are not attractive. Removing and transporting a large housing is slow and expensive, welding adds heat that can distort it, and a replacement may take months to arrive. For many plants and vessels, the housing cannot leave the machine without shutting down a whole line.
This article walks through how a worn bearing housing can be restored on site using Brush Plating,
based on a repair procedure we have used for large housings.
The Problem
Bearing housings and bearing pockets are precision surfaces. They have to hold the bearing shell or bearing outer ring at an exact size and alignment. Over time, they can suffer from:
- Scorelines, caused by a spinning or seized bearing
- Pitting and corrosion, from moisture or contamination
- Fretting wear, from a bearing that has loosened in its seat
Once the bore is out of size, the bearing no longer sits properly. Left alone, this leads to vibration, overheating, and repeat bearing failures.
Why Repair In Situ?
Repairing the housing in place, without removing it from the machine, offers real advantages:
- Less downtime. There is no need to dismantle and transport a large, heavy component.
- Alignment is preserved. The housing stays in its installed position, which makes it easier to restore the original alignment.
- Low heat. The Brush Plating process runs at a maximum temperature of 65°C, so there is no risk of the distortion that welding can cause.
- Targeted repair. Only the damaged pockets are treated. The rest of the housing is masked off and untouched.
The Repair Process
The procedure below is based on our standard in-situ method. Some steps are carried out by Sterling, and others by the customer or their contractor, so responsibilities are clear from the start.
1. Confirm the repair is viable (customer). Before any work begins, dye-penetrant, dimensional, and alignment checks are performed to establish the extent of the damage and confirm the housing can be repaired.
2. Clean and prepare the surface. The area is degreased with detergent and water. Scorelines and pitting are then lightly hand-ground to widen the scores, but not to deepen them, which leaves a clean surface for the plating to bond to.
3. Mask and protect.
Adjacent surfaces and reference areas are masked, so plating goes only where it is needed. In the photos, green tape and plastic sheeting protect the surrounding housing.
4. Electrolytic cleaning and etching. An alkaline electrolytic clean removes trace oil. An electrolytic acid etch then brings out impurities on the metal surface, followed by desmutting. This step is critical for adhesion.
5. Nickel bonding layer. A thin nickel layer, around 5 microns thick, is applied electrolytically. It acts as a bonding layer between the base metal and the copper that follows.
6. Copper build-up. Copper is applied to the required thickness, with enough extra material (overbuild) for machining. In this procedure, the overbuild allowance is 0.100 mm.
7. Check thickness and adhesion.
The copper thickness in the pockets is measured without damaging the surface and recorded, to confirm there is enough material for line boring. A non-destructive adhesion test using a high-tack adhesive tape is carried out on several areas and recorded before handover.
8. Line boring (customer). The customer or their contractor machines the plated pockets back to the original size and alignment. We provide machining guidance for plated copper, summarized below.
9. Nickel cap. After boring, a thin nickel cap of about 5 microns is applied as a cosmetic and corrosion-resistance layer. No further machining is needed.
10. Final checks (customer). The customer performs final dimensional and alignment checks before the machine returns to service.
Machining Guidance for Plated Copper
Copper is soft, so how it is cut matters. Our guidance for line boring is:
- Cutting speed of 60 feet (18.3 m) per minute or less
- Very light cuts, starting at 0.0005 inch (12.5 microns), until the whole deposit surface is being cut
- Sharp carbide or ceramic tool bits
- Plenty of coolant
- Where possible, cut from the center of the deposit outwards to the edge
Why It Works
Several things make this approach suitable for bearing housings:
- Controlled build-up. Metal is applied in layers, with thickness measured before the housing goes for machining.
- Strong bonding. Careful cleaning, electrolytic etching, and a nickel bonding layer prepare the surface so the copper stays attached. Adhesion is checked and recorded before machining.
- Clear division of responsibility. Inspection and machining are handled by the customer or their contractor, and plating by us, with every step documented.
- Reduced risk. No heat distortion, no need to move the housing, and no long wait for a replacement.
When Repair Is Not the Right Answer
In-situ Brush Plating is not suitable for every housing. Replacement should be considered when the housing is cracked or structurally damaged, when wear is too deep for a surface build-up to be practical, or when the base material is not sound enough to hold a bonded layer. The initial dye-penetrant, dimensional, and alignment checks are there to settle this before any plating begins.
Have a Worn Bearing Housing?
If you have a bearing housing with scored, pitted, or worn pockets, send us:
- Clear photos of the damage, with a scale in the frame
- The measured and specified bore sizes
- Any dye-penetrant, dimensional, or alignment reports you already have
- The machine type, location, and how quickly it needs to return to service
Our team can tell you whether the housing is a candidate for in-situ Brush Plating repair and what the process would involve.